Wet Oxide Etch

INTRODUCTION:

Buffered oxide etch (BOE) is used to remove SiO2. BOE is a very selective etch, meaning thatit stops at the silicon and does not etch further. The etch may be used for in many steps, such as exposing the active region near the beginning of a process or defining contact holes at the end.

SAFETY:

BOE consists of HF acid at high concentration levels (about 10X greater than the oxide strip in the RCA clean).  HF acid is very dangerous and HF burns are particularly hazardous. An insidious aspect of HF burns is that there may not be any discomfort until long after exposure. These burns are extremely serious and may result in tissue damage. If you contact HF, flush the area well and be sure to work under and around your finger nails. Finger nails and cuticles are the classic areas where people receive burns, having washed off the HF without washing under their nails. If washed off within a few minutes of exposure, HF may do no harm. Remember, HF may not produce any burning sensation until after it has already done damage. All HF burns should be looked at by a physician.

Acid protective gear MUST be worn when working at this sink. A lab coat, goggles, acid-proof gloves (atop the normal clean room gloves), and an acid face mask (with the face shield DOWN) worn over safety glasses, are all required. ALWAYS know thelocation of the nearest eye wash and safety shower.

PROCEDURE:

I. Preparation of Solution  - Will be done by staff prior to lab.

Chemicals
A. DI Water (DIH2O)
B. Hydrofluoric Acid (HF)
C. Ammonium Flouride (NH3F)

A. Mix 400 g of Ammonium Flouride with 600 ml of water.
B. Carefully mix Ammonium Flouride Solution with HF in a 6:1 ratio.

Overall reaction for etching SiO2 with BOE:
SiO2 + 4HF ==> SiF4 + 2H2O
where a buffering agent, ammonium fluoride (NH4F), is added to maintain HF concentration and to control pH (to minimize photoresist attack):
Buffering reaction:  NH4F <==> NH3 + HF.

II. Etching Procedure

A. Mount wafer on teflon wand.
B. The etch rate for BOE is about 1000�/min. Estimate the appropriate etch time required base on your known oxide thickness.
C. Immerse wafer in BOE for the desired time. When complete remove and rinse well with DI water, and blow dry with nitrogen.
D. If the etch was complete, then BOE and water should bead or "dewet" off the wafer backside. Why is that?
E.After the etch is complete, inspect the wafers under the microscope. The exposed patterned regions should appear to be silicon colored (white or metallic colored). If the exposed patterned regions still appeared colored, the wafers should be returned to the BOE. 
F. Strip off the photoresist using an oxygen plasma in the RIE.
G. Using the Surface Profiler characterize the topography of your wafers to ensure that your ecth was complete.

 

http://inside.mines.edu/fs_home/cwolden/chen435/wetoxide.html

 

MSDS : http://www.jtbaker.com/msds/englishhtml/B5636.htm

?

List of Articles
번호 분류 제목 글쓴이 날짜 조회 수
공지 회사 목록 모아레 2011.02.07 52057
공지 메모 연락처 목록 모아레 2010.08.05 26987
공지 메모 유용한 사이트 모아레 2010.02.25 39811
공지 메모 메모 정리 (미완) 모아레 2009.10.30 24145
공지 메모 연구실 장비 목록 모아레 2009.09.30 30812
공지 메모 주문, 구입 리스트 모아레 2009.09.21 24820
공지 메모 To do list, Short Memo 모아레 2009.08.20 27052
52 메모 메일서버 접속문제 해결 모아레 2009.09.25 10065
51 메모 ZnO Nanowire COMSOL Simulation 참고 모아레 2010.09.11 9911
50 메모 Keywords 모아레 2009.09.11 9892
49 자료 전자 부품 모아레 2010.01.26 9844
48 자료 Litho 관련 용어 정리 모아레 2009.07.08 9752
47 메모 Vacuum can 제작할 때 참고할 것. 모아레 2009.08.19 9732
46 자료 Coplanar Waveguide 모아레 2010.01.31 9707
45 메모 옥스포드장비에 연결할 어댑터 맡겨놨음 모아레 2009.07.15 9700
44 메모 연구실 공유기, 프린터 공유 설정 모아레 2009.07.19 9682
43 자료 반도체 기초자료 - Lithography 등 모아레 2011.01.17 9672
42 메모 회식 자리 모음 모아레 2009.11.07 9586
41 자료 오실로스코프의 이해와 올바른 사용법 모아레 2009.09.13 9576
40 자료 Noise (in audio amplifiers) 모아레 2010.10.08 9568
39 메모 중전 Windows XP EN 시디키 모아레 2010.01.25 9497
38 자료 COMSOL 시뮬레이션 참고자료 모아레 2009.07.30 9480
37 메모 클린룸 관련 사이트 모아레 2009.09.21 9447
36 자료 Anodic Aluminum Oxide(AAO) 연구 분야 모아레 2010.08.21 9355
35 자료 Network Analyzer 모아레 2010.08.11 9339
34 기타 how to confirm the impedance of the microstrip? 모아레 2010.07.10 9329
33 메모 Endnotes 학교에서 다운받는 곳 모아레 2009.09.17 9301
Board Pagination Prev 1 ... 2 3 4 ... 5 Next
/ 5